Skip to content
Battery Engineering Academy

Batteries that move us · Beginner · 300 min

Why fast charging slows down near full

Why "10 to 80 % in 20 minutes" is the number every fast charger advertises, why the last 20 % takes so long, and why charging a cold battery fast is risky.

By the end of this lesson you can

  • Describe the constant-current, constant-voltage (CC-CV) charging profile
  • Explain, using OCV and internal resistance, why the charging current must fall as the cell fills
  • Calculate ideal charging times for an SOC window and compare the fast and slow parts of a charge
  • Explain why fast charging a cold battery is limited, and the risk of lithium plating

Before this: Why your phone battery wears out · Power versus energy: W, Wh, kWh

Fast-charging curves have a common shape: high power at first, then a steady decline as the battery fills. The decline, called the taper, is not a limitation of the charger. As the cell approaches full, its voltage rises towards the maximum allowed, and the current must fall to stay below that limit while also avoiding lithium plating. This is why charging from 10 to 80 % is quick and the last 20 % is slow.

Study plan · two days

  1. Day 1 (about 2.5 h): Why charging slows down. The bottle-filling picture, the constant-current constant-voltage profile, and worked examples. Practice drills and the knowledge check.
  2. Day 2 (about 2.5 h): Planning a charging stop. Time in a window at constant rate, the current limit near full, and why stopping at 80 % is often faster. Homework and further reading.

Filling a bottle at a tap

Intuition

Imagine filling a bottle with a narrow neck from a powerful tap. At first, you open the tap fully: the bottle fills fast. As the water nears the neck, you must slow down or it will overflow and splash. The last part fills slowly, however strong your tap is.

A lithium-ion cell has a "neck" too: a maximum voltage it must never exceed (C06-L03). Charging pushes the terminal voltage up, and the nearer the cell is to full, the closer that voltage gets to the limit. To avoid crossing it, the charger has to keep turning the current down.

The CC-CV profile

Engineering

Almost all lithium-ion charging follows two phases:

  1. Constant current (CC): the charger supplies its maximum allowed current. The cell's voltage rises steadily.
  2. Constant voltage (CV): once the terminal voltage reaches the maximum (for example 4.2 V for many NMC cells), the charger holds the voltage there. The current falls on its own as the cell fills, and charging ends when the current drops below a small cut-off.

Why must the current fall? While charging, the terminal voltage is the OCV plus the voltage drop across the internal resistance (C06-L01):

V=VOCV(SOC)+I R0V = V_\text{OCV}(\text{SOC}) + I\,R_0

To keep V≤VmaxV \le V_\text{max}, the current can be at most:

Imax=Vmax−VOCVR0I_\text{max} = \frac{V_\text{max} - V_\text{OCV}}{R_0}
  • VmaxV_\text{max}: maximum allowed cell voltage, in V
  • VOCVV_\text{OCV}: open-circuit voltage at the present SOC, in V; it rises as the cell fills
  • R0R_0: internal resistance, in Ω

As SOC rises, VOCVV_\text{OCV} climbs towards VmaxV_\text{max}, so the "headroom" shrinks and ImaxI_\text{max} falls. This simplified model (resistance only, no slower dynamics) already shows the taper. Real chargers also limit current for heat and lifetime reasons (C06-L09).

Solved examples

Worked example

Example 6.1: the taper, from our simplified cell model

Our illustrative 5 Ah NMC cell model has R0=25 mΩR_0 = 25\ \text{m}\Omega and Vmax=4.2 VV_\text{max} = 4.2\ \text{V}. Its OCV curve gives:

SOCOCV (model)Max current (4.2−OCV)/0.025(4.2 - \text{OCV})/0.025C-rate
50 %3.70 V20 A4C
80 %3.95 V10 A2C
90 %4.05 V6 A1.2C
95 %4.115 V3.4 A0.7C

With a charger limited to 10 A (2C), the cell charges at full current up to about 80 %. After that, the voltage limit forces the current down, which is exactly where the screen shows the charge rate dropping. (Illustrative model, not a real cell; C12 adds the dynamics this ignores.)

Worked example

Example 6.2: why the last 20 % takes so long

Ideal time to move through an SOC window at a constant C-rate: t=(ΔSOC/100)×60/Ct = (\Delta\text{SOC}/100) \times 60/C minutes.

  1. 10 % → 80 % at 2C: 0.70×60/2=21 min0.70 \times 60/2 = 21\ \text{min}
  2. 80 % → 100 % at an average of about 0.5C during the taper: 0.20×60/0.5=24 min0.20 \times 60/0.5 = 24\ \text{min}

The last 20 % takes longer than the first 70 %. That is why fast-charging claims quote 10–80 %, and why on a road trip it is often quicker to stop twice for short charges than once to 100 %.

Worked example

Example 6.3: charging when cold

In the cold, the cell's resistance rises. Suppose R0R_0 doubles to 50 mΩ (an illustrative figure).

At 50 % SOC: Imax=(4.2−3.70)/0.050=10 AI_\text{max} = (4.2 - 3.70)/0.050 = 10\ \text{A}, half of the 20 A it could take when warm. The taper starts much earlier and the whole charge is slower.

There is a second, more serious reason. When a cold cell is charged fast, lithium can deposit as metal on the surface of the graphite instead of moving inside it. This lithium plating permanently reduces capacity and, in severe cases, can create safety risks. That is why EVs warm their batteries before fast charging and why chargers sharply limit current at low temperature (C15, C20).

Worked example

Example 6.4: what “10–80 % in 21 minutes” means for an EV

A car with a 60 kWh usable pack charges from 10 % to 80 % in 21 minutes.

  1. Energy added: 0.70×60=42 kWh0.70 \times 60 = 42\ \text{kWh}
  2. Average power: 42/(21/60)=120 kW42 / (21/60) = 120\ \text{kW}

The charger's peak power is higher than this average, and the power after 80 % is much lower. Both the car's battery and the charger set the limit; the lower one wins.

Simulator

Maximum charge current (A) against Open-circuit voltage (V), rises as the cell fillsMaximum charge current (A) plotted against Open-circuit voltage (V), rises as the cell fills from 3.5 to 4.18. Current settings: Voltage limit (V) 4.2, Cell resistance R₀ (mΩ) 25. At Open-circuit voltage (V), rises as the cell fills = 4.05, the value is 6 A.0102030403.63.84Open-circuit voltage (V), rises as the cell fillsMaximum charge current (A)6 A
The current that keeps the terminal voltage at the limit, (V_max − OCV)/R₀. As OCV rises the allowed current falls: this is the taper. Simplified ohmic-only model; Python-verified formula.

Common mistakes

  • "The charger is slowing down because it is faulty." The taper is designed in: it protects the cell from overvoltage and plating.
  • Quoting 0–100 % time as "fast-charging time". The taper makes the last part slow, so the industry compares 10–80 %.
  • Fast charging a very cold battery. It is limited for good reason: plating risk.
  • Thinking a bigger charger always helps. If the battery's limit is lower, the extra charger power is unused.

Practice

Numbers change each time you press New values. Answers within about 1 % are accepted.

  1. D1

    A cell has OCV 3.85 V, a maximum voltage of 4.2 V and R0 = 20 mΩ. Using the R0-only model, what is the largest charging current that keeps it at or below the maximum, in A?

    A
  2. D2

    Ideally, how long does it take to charge from 10 % to 60 percentage points higher at a constant 1.5C, in minutes?

    min
  3. D3

    During the taper from 80 % to 100 %, the average rate is only 0.5C. Ideally, how long does that last 20 % take, in minutes?

    min
  4. D4

    On a cold morning, a cell's R0 has risen to 50 mΩ. Its OCV is 3.7 V and its maximum is 4.2 V. What is the R0-limited charging current, in A?

    A
  5. D5

    A charger is limited to 1C for a 4.8 Ah cell. What is that current limit, in A?

    A

Check your understanding

1. What happens in the CV (constant-voltage) phase of CC-CV charging?
2. Using V = OCV + I·R0, why must the charging current fall as the cell fills?
3. Why do fast-charging claims usually quote 10–80 % rather than 0–100 %?
4. What is lithium plating?
5. A cell charges from 10 % to 70 % at a steady 2C. Ideally, how long does that take?

Time in a window

Worked example

Example 6.5: 10 to 80 % at 2C

  1. Ideal time at a constant 2C: 70/100×60/2=2170/100 \times 60/2 = 21 minutes
  2. Near 80 %, with OCV 4.05 V, limit 4.2 V and R0=25R_0 = 25 mΩ, the allowed current is (4.2−4.05)/0.025=6(4.2 - 4.05)/0.025 = 6 A, or 1.2C for a 5 Ah cell

The charge is therefore not at 2C all the way; real times are longer than the ideal figure, and the final 20 % takes longer still as the current keeps falling.

Planning a fast-charging stop

  1. 1Arrive low

    Below about 20 %: charging power is highest.

  2. 2Charge to ~80 %

    Most energy per minute.

  3. 3Leave

    The last 20 % takes disproportionately long.

  4. 4Warm battery

    Precondition in winter for higher current.

Maths· Why the current falls exponentially in the CV phase

In the constant-voltage phase the terminal voltage is held at VmaxV_\text{max}, so I=(Vmax−U)/RI = (V_\text{max} - U)/R, where UU is the open-circuit voltage. As charge enters, UU rises approximately in proportion, dU/dt=kIdU/dt = k I for a local slope kk (V per Ah). Substituting gives dI/dt=−(k/R)IdI/dt = -(k/R)I, so the current decays exponentially with time constant R/kR/k. A flatter OCV curve (small kk) gives a slower decay, which is one reason LFP cells taper differently from NMC.

Homework

Homework · answers not provided

  1. Compute the ideal time from 20 to 80 % at 1.5C and from 80 to 100 % at 0.5C. Which is longer per percent?
  2. For R₀ = 15 mΩ and 40 mΩ, compute the allowed current at OCV = 4.10 V with a 4.2 V limit.
  3. Explain why charging a cold battery is slower even with the same charger.
  4. Plan a 400 km trip in an EV with 60 kWh usable and 160 Wh/km, choosing when to stop and to what SOC. State your assumptions.

Further reading

Further reading

  • G. L. Plett, Battery Management Systems, Volume II, Artech House, 2016. Charge control and power limits.
  • J. Vetter et al., J. Power Sources 147 (2005). Ageing effects of charging conditions.

Key takeaways

  • Lithium-ion charges with CC-CV: full current first, then constant voltage while the current tapers.
  • The taper follows from V=VOCV+IR0≤VmaxV = V_\text{OCV} + IR_0 \le V_\text{max}: as the OCV rises, the allowed current falls.
  • The last 20 % can take as long as the first 70 %, which is why "10–80 %" is the standard claim.
  • Cold raises resistance and plating risk, so cold cells must be warmed or charged slowly.
  • 10–80 % at 2C takes 21 minutes ideally; the current limit near full makes the real time longer.
  • Allowed current = (V_max − OCV)/R: higher resistance or a fuller cell means less current.
  • Next: grid storage, where cost and cycle life matter more than energy density.

Sources for this lesson are listed on the References page.